Guangdong Chair Factory Notes Production floor, Longjiang · Foshan

Factory Notes › Wooden Bar Stools

Timber Drying and Moisture Control for Bar Stools

Kiln schedule, the 8-12 percent band, case-hardening and why most joint failures in bar stools are actually moisture failures.

Updated 2026-11-14Longjiang, Foshan16 min read

Kiln schedule, the 8-12 percent band, case-hardening and why most joint failures in bar stools are actually moisture failures.

These notes come off the production floor in Longjiang, Foshan. The current wholesale wooden bar stools range is on the main site, with a specification page for every model in it.

Why the kiln is the most important room in the factory

Most seating failures blamed on joinery are actually moisture failures. Timber that leaves a kiln too wet shrinks after it is made into a frame, and the glue line opens. The joint was fine; the water content was not.

A stool is a tall, narrow object with a footring, and the moisture problems in this category show up in the column and the ring rather than in the seat. A column that dried unevenly bows, and a bow is obvious the moment someone sits on it.

We dry to 8 to 12 percent and meter every batch. The reading is recorded against the batch number and printed on the packing list, so it can be checked at destination.

Height decides everything: 650 mm seat for a 900 mm bar top, 750 mm for a 1050 mm counter. Get it wrong by 50 mm and the sitter either perches or cannot reach the top. Kitchen islands in apartments are the fastest growing part of this category.

The schedule

A kiln charge runs 15 to 25 days depending on species and section thickness, stepping temperature up and humidity down in stages. Rushing it by raising temperature early produces case-hardening: the outside of the board dries and locks while the core is still wet, and the board moves later, inside a finished chair.

The column and the footring are the thick sections here: a 45 to 60 mm column blank, a ring formed from 25 to 30 mm stock, seat blanks at 25 to 30 mm. On the swivel models the column is bought in as tube and machined to fit the mount.

A stool column is a thick section and a footring is a bent one, and both come out of the same charge as thinner seat blanks. That is exactly the case where one schedule delivers two moisture contents, so the thick stock is dried separately.

StageTemperatureDurationPurpose
Pre-heating40-50 °C, high humidity1-2 daysWarm the charge through
Main drying55-70 °C stepped10-18 daysDown to 12-14%
Equalising70-75 °C, low humidity2-4 daysEven out the core
ConditioningSteam injection1-2 daysRelieve case-hardening
Cool and meterAmbient1 dayVerify 8-12% before release

Kiln schedule

Defects we reject for

End checking, collapse, honeycombing, sticker stain and fungal discolouration. Any of these disqualify a board from a frame component. They are cheap to reject at the kiln and expensive to discover after assembly. Wooden Bar Stools use the same graded stock as every other model we build.

A stool is seen from below as often as from above — the underside of the seat and the footring sit at eye level for anyone at the bar. Both get the same three-grit sequence as the visible faces, and the ring is finished before it is welded.

Equilibrium, and what it means for your market

Timber settles at the moisture content the surrounding air dictates. A frame that arrives at 10 percent into a heated Nordic restaurant at 30 percent relative humidity will drop towards 6 percent and shrink as it does. That movement is normal and it is why we hold the band, seal end grain, and specify a joint that tolerates it.

Stool columns are thick and they respond slowly to a change in humidity, which helps: a column that arrives at 10 percent will not fall to 6 percent in a week. The seat, at 25 mm, will. That mismatch inside one product is why components are metered separately.

Species behave differently in the kiln

Ash — around 70% of what we run — dries steadily and holds its colour if the schedule is respected. Rubberwood, the other 30%, dries quickly and evenly and is the most forgiving charge in the yard. Oak is slow and prone to checking if pushed, and beech dries fast but collapses if the temperature goes up too early; both are custom runs for us. The schedule is written per species, not per thickness, and the two get confused constantly.

Most stools here run a wood seat on a wood or metal column, so the timber in the charge is seat stock — ash on roughly 70% of the programme, rubberwood on the rest. Plated metal components arrive finished and are not part of the moisture conversation at all.

What bar stools demand from the kiln

A stool carries its load differently from a chair. The seat is high, the base is narrow relative to the height, and the footring takes a sideways kick every time someone climbs on or pushes off. That is why the ring on our stools is a welded closed section joined to the column, not a ring screwed into a leg.

The critical junction is where the column meets the seat mount and where the footring meets the column. On a swivel model the gas lift is a bought-in component and we test the assembly, not just the frame: a lift rated for office duty is not the same part as one rated for a bar that runs twelve hours a day.

What happens after the kiln

Dried stock is held in a covered, conditioned store until it is machined. Leave it in an open yard through a Foshan wet season and it will take water back up within days, which undoes the schedule. This is the step most factories skip and the reason a moisture reading taken at packing matters more than one taken at the kiln.

We meter at both. If the two disagree, the charge goes back before it reaches the machining line.

Seat blanks for stools are small and they take water back quickly if they stand in an open yard. They move from the kiln to a covered store and are machined within the week, because a 25 mm blank has very little reserve.

Stools pack small — 0.08 to 0.12 m³ for two — so the freight per piece is the best in the catalogue and a 40HC holds a lot of them. MOQ is 6 pieces per model.

Which models this applies to

There are 86 models in this category: 44% run on a solid wood frame and 33% carry an upholstered or soft cover, so the moisture discipline applies to different components in different proportions.

Three of them as they stand today: A10037 (Solid Wood, MOQ 6 pcs), by-62565 (Leather/Velvet/Fabric, MOQ 6 pcs), A001 (100% Solid Wood, MOQ 2 pcs).

What moisture damage looks like on bar stools

The three returns we see: footring welds cracking after a season, swivel mechanisms that lose their gas, and seat pads compressed flat at the front edge. All three are specifiable — a closed-section ring, a contract-rated lift, and a 35 kg/m³ foam.

Beyond the frame test a stool gets a stability check at height and a footring load test: push the ring sideways with the stool loaded and it must not deform. Swivel models are cycled, not just sat on.

Reading a moisture meter properly

Take three readings along a blank and average them, and correct for timber temperature. Pin meters, not pinless ones — and the reading that counts is the one taken at packing, not the one taken at the kiln.

Questions

What moisture content do you ship at?

8 to 12 percent, metered per batch, with the reading recorded on the packing list.

Does the schedule change for this category?

A stool column is a thick section and a footring is a bent one, and both come out of the same charge as thinner seat blanks. That is exactly the case where one schedule delivers two moisture contents, so the thick stock is dried separately.

Can I specify a tighter band?

Yes - say the target on the order and the charge is scheduled to it.

Does the schedule change for bar stools?

A stool carries its load differently from a chair. The seat is high, the base is narrow relative to the height, and the footring takes a sideways kick every time someone climbs on or pushes off. That is why the ring on our stools is a welded closed section joined to the column, not a ring screwed into a leg.

What goes wrong on bar stools if the moisture content is off?

The three returns we see: footring welds cracking after a season, swivel mechanisms that lose their gas, and seat pads compressed flat at the front edge. All three are specifiable — a closed-section ring, a contract-rated lift, and a 35 kg/m³ foam.